ACC SURAKSHA is the new brand name for a specially blended cement, produced by inter grinding higher strength ordinary portland cement clinker with high quality processed fly ash- based on norms set by ACC’s own R & D division. This makes ACC Suraksha  a ‘value added product’ with long-standing hydraulic binding properties- not found in ordinary cements. Which means construction that will last for generations when you build with ACC Suraksha.

CHARACTERISTICS OF ACC SURAKSHA

  • Reduction in heat during hydration, as a result reduction in cracking and extensibility.
  • Freedom form segregation and less bleeding.
  • Improvement in workability.
  • Alkali aggregates reaction is inhibited.
  • Improved resistance to sulphate attack.
  • Improved long term strength over OPC.
APPLICATIONS OF ACC SURAKSHA
  • All construction for plain and reinforced work.
  • Mass constructions.
  • Bridge piers.
  • Large foundation work.
  • All marine concrete structures such as docks, harbours, jetties.
  • Industrial plants.

WORKS TEST CERTIFICATE
 
   
Results
11 Requirements as per IS:1489(Part-1)-1991
 1  CHEMICAL COMPOSITION:    
  % Soluble Silica    
  % Alumina    
  % Iron Oxide     
  % Magnesia
1.0
Not more than 6.0%
  % Insoluble Residue
11.2
Not more than 6.0%[X+4.0(100-X)/100]
X is %Pozzolana in PPC
  % Sulphur calculated as SO3
2.2
Not more than 2.5 if C3A is 5.0 or less & 
Not more than 3.0 if C3A is more than 5.0
  % Loss On Ignition
2.4
Not more than 5.0%
  % Chloride
0.012
 
  % Alkalies as Na2O    
       
 2  FINENESS    
  Specific Surface (m2/kg)
352
Not less than 300 
       
 3  COMPRESSIVE STRENGTH (MPa):    
  at  3-Days
36.0
Not less than 16
       7-Days
44.5
Not less than 22
       28-Days
56.5
Not less than 33
       
 4  SETTING TIME:    
  Initial (Minutes)
140
Not less than 30
  Final (Minutes)
215
Not less than 600
       
 5  SOUNDNESS    
  Le-Chatelier Expn (mm)
1.0
Not more than 10 mm
  Autoclave Expn. (%) 
0.06
Not more than 0.6%
       
 6 a) Normal Consistency (%)
27.2
 
  b) Temp.during Testing (0C) 
27+/-2
 
  c) % POZZOLANA MATERIAL USED
12.0
 

Comparison between SRPC and SURAKSHA

PROPERTIES SRPC SURAKSHA
1. CHEMICAL COMPOSITION
C3A Percent by Mass
2.2
2.0
2. FINENESS
Specific Surface m2/kg
315
361
3. SOUNDNESS
Lechatliers Expansion (mm)
1.50
1.0
Autoclave Expansion (%)
0.008
0.03
4. SETTING TIME
Initial (Minutes)
130
155
Final (Minutes)
180
210
5. COMPRESSIVE STRENGTH (MPa)
3 days
26.5
31.0
7 days
37.0
40.5
28 days
50.5
50.5
Top of Page

cements, cement stockists, acc cement, larsen & tourbro cement, vasavadatta cement, sika, orient cement, grasim, acc suraksha, ordinary portland cement, sulphate resisting portland, ready mixed concrete, acc shrinkkomp, accoproof, acc bulk cement, acc samrat, mumbai, india, indian, span cements, span, refactories